            O, N determination in titanium samples

            閱讀:5734      發(fā)布時間:2015-05-15
            分享:
              Suitable analyzers
            n ON 900
            n ONH 2000
            Used accessories
            n Inner graphite crucibles (90180)
            n Outer graphite crucibles (90185)
            n Nickel basket (90250) or AR 2344
            n Suitable calibration material (NIST or other)
            Settings
            n Comparator level: 20 mV
            n Minimum time: 15 sec
            n Maximum time: 3:00 min
            n Post waiting: 30 sec
            n Base line deviation: 200 mV;
            Step: 16 mV; Time: 10 sec
            n Mode: continuous
            n Outgas
            Time: 45 sec
            Power: 6 kW
            n Time
            Purge: 20 sec
            Stability: 45 sec
            n Integration delay
            IR cell: 2 sec
            TC cell: 10 sec
            n Analyse (1)
            Time: 75 sec
            Power (1): 6 kW
            Power (2): 6 kW

            Sample preparation
            Make sure that the surface of the titanium is free
            from contaminations; otherwise clean the sample with
            acetone p.a. and let dry at atmosphere.
            Procedure
            n Prepare ELTRA analyzer (exchange anhydrone,
            sodium hydroxide, copper oxide when necessary),
            clean furnace, sample drop mechanism, electrode tip
            n Run three blanks with empty crucibles
            n Calibrate the analyzer with suitable calibration
            material (NIST or other)
            (1) Fill one empty inner crucible (90180) in one outer
            crucible (90185) and place them on the electrode
            tip, close furnace (F2 Button)
            (2) Weigh calibration material and give it into a nickel
            basket (90250 or AR2344)
            (3) Place nickel basket with calibration material or sample
            in the sample drop mechanism and start analysis
            (F5 Button)
            After analysis give the inner crucible into waste and
            fill in a new one. The outer crucibles can be used
            approximay 10 times.
            Repeat steps (1) – (3) at least three times;
            Mark the results and use the calibration function in the
            software.


            提供商

            弗爾德(上海)儀器設(shè)備有限公司

            下載次數(shù)

            196次

            資料大小

            370KB

            資料類型

            PDF 文件

            資料圖片

            --

            瀏覽次數(shù)

            5734次

            會員登錄

            請輸入賬號

            請輸入密碼

            =

            請輸驗(yàn)證碼

            收藏該商鋪

            標(biāo)簽:
            保存成功

            (空格分隔,最多3個,單個標(biāo)簽最多10個字符)

            常用:

            提示

            您的留言已提交成功!我們將在第一時間回復(fù)您~
            在線留言
            涟水县| 陵川县| 洱源县| 仙桃市| 扎鲁特旗| 镇康县| 永寿县| 托克托县| 云林县| 新巴尔虎右旗| 东乌珠穆沁旗| 昭觉县| 毕节市| 横峰县| 台北市| 固镇县| 庆元县| 南昌县| 郴州市| 丁青县| 尼玛县| 慈溪市| 三明市| 孝感市| 当涂县| 白沙| 迭部县| 泾阳县| 承德县| 图木舒克市| 酒泉市| 济南市| 盈江县| 汝城县| 左权县| 锦屏县| 崇左市| 郁南县| 莆田市| 定西市| 北流市|