              Suitable analyzers
            n ON 900
            n ONH 2000
            Used accessories
            n Graphite crucibles (90190)
            n Suitable calibration material (NIST or other)
            Settings
            n Comparator level: 5 mV (low oxygen);
            20 mV (other)
            n Minimum time: 15 sec (oxygen);
            35 sec (nitrogen)
            n Maximum time: 3:00 min
            n Post waiting: 20 sec
            n Base line deviation: 20 mV;
            Step: 16 mV; Time: 10 sec
            n Mode: continuous
            n Outgas
            Time: 45 sec
            Power: 5 kW
            n Time
            Purge: 15 sec
            Stability: 45 sec
            n Integration delay
            IR cell: 2 sec
            TC cell: 10 sec
            n Analyse (1)
            Time: 40 sec
            Power (1): 4 kW
            Power (2): 4 kW

            Sample preparation
            Make sure that the surface of the steel is free from
            contaminations; otherwise clean the sample with
            acetone p.a. and let dry at atmosphere.
            Procedure
            n Prepare ELTRA analyzer (exchange anhydrone,
            sodium hydroxide, copper oxide when necessary),
            clean furnace, sample drop mechanism, electrode tip
            n Run three blanks with empty crucibles
            n Calibrate the analyzer with suitable calibration
            material (NIST or other)
            (1) Place empty crucible (90190) on the electrode tip,
            close furnace (F2 Button)
            (2) Weigh calibration material (usually pins)
            (3) Place calibration material in the sample
            drop mechanism and start analysis (F5 Button)
            Repeat steps (1) – (3) at least three times;
            Mark the results and use the calibration function in
            the software.


            提供商

            弗爾德(上海)儀器設(shè)備有限公司

            下載次數(shù)

            151次

            資料大小

            363.3KB

            資料類型

            PDF 文件

            資料圖片

            --

            瀏覽次數(shù)

            2736次

            產(chǎn)品展示

            會員登錄

            請輸入賬號

            請輸入密碼

            =

            請輸驗證碼

            收藏該商鋪

            標簽:
            保存成功

            (空格分隔,最多3個,單個標簽最多10個字符)

            常用:

            提示

            您的留言已提交成功!我們將在第一時間回復您~
            在線留言
            洪雅县| 密山市| 大方县| 论坛| 射阳县| 莎车县| 日土县| 灵寿县| 中西区| 封开县| 布拖县| 海南省| 治县。| 巫山县| 正安县| 沙河市| 阳山县| 寿阳县| 太白县| 葫芦岛市| 北碚区| 阿拉善左旗| 克拉玛依市| 定安县| 黔东| 石屏县| 二连浩特市| 玉屏| 洪江市| 翼城县| 兰溪市| 鄂尔多斯市| 甘肃省| 杭锦旗| 双桥区| 灵丘县| 巫山县| 石嘴山市| 大港区| 渑池县| 东乡县|